Spring Steel Grades and Materials: A Selection Guide
Author: Jenny Xu
Published: Nov 10, 2026
Updated: Nov 10, 2026
Spring steel is a high-carbon or alloy steel with a high yield strength, so it can deflect a long way and return to shape. The most common grades are music wire (ASTM A228), oil-tempered wire (A229), chrome-vanadium (A231), chrome-silicon (A401) and stainless steel 302/304 (A313). The choice depends mainly on stress, temperature and corrosion.
Common spring materials compared
| Material | Standard | Shear modulus G (GPa) | Typical upper limit (°C) | Typical use |
|---|---|---|---|---|
| Music wire | ASTM A228 | 81.7 | 120 | Small, high-stress springs at room temperature |
| Hard-drawn carbon | ASTM A227 | 80.0 | 120 | Low-cost, lightly cycled springs |
| Oil-tempered carbon | ASTM A229 | 77.2 | 150 | General springs in larger wire |
| Chrome-vanadium | ASTM A231 | 77.2 | 220 | Shock loading, die springs |
| Chrome-silicon | ASTM A401 | 77.2 | 245 | High stress and fatigue duty |
| Stainless 302/304 | ASTM A313 | 69.0 | 260 | Corrosive environments |
| 17-7 PH stainless | ASTM A313 | 75.8 | 315 | Corrosion resistance with higher strength |
| Phosphor bronze | ASTM B159 | 41.4 | 95 | Conductive springs and contacts |
| Beryllium copper | ASTM B197 | 44.8 | 205 | Conductive springs needing higher strength |
Temperature limits are typical published values for ordinary service. The real limit depends on stress and on how much relaxation the application can accept.
Cold-coiled and hot-coiled steels
Cold-coiled springs are usually wound from wire that is already hardened, then stress-relieved. Hot-coiled springs are wound from bar at about 850–950 °C and then quenched and tempered. Common hot coil spring steels include 60Si2Mn, 51CrV4, 54SiCr6 and SAE 5160 and 9254. Grades such as 65Mn and 60Si2Mn are widely used under Chinese GB standards.
Stainless steel springs
Stainless steel 302/304 has a shear modulus about 13% lower than carbon spring steel, 69 GPa against about 79 GPa. A stainless spring with the same dimensions therefore has about 13% less rate, so the wire or coil count must change if the force has to stay the same. Grade 316 resists chlorides better but is usually lower in strength. 17-7 PH keeps more strength at temperature.
Nearest international equivalents
| Material family | ASTM | EN | JIS |
|---|---|---|---|
| Music wire | A228 | EN 10270-1 DH | G3522 SWP |
| Oil-tempered carbon | A229 | EN 10270-2 FDC, TDC | G3560 SWO |
| Chrome-silicon | A401 | EN 10270-2 FDSiCr | G3561 SWOSC-V |
| Chrome-vanadium | A231 | EN 10270-2 FDCrV | G3561 SWOCV-V |
| Stainless 302 type | A313 | EN 10270-3 1.4310 | G4314 SUS302 |
These are close equivalents, not identical specifications. Tensile ranges differ by size and standard, so confirm the grade against the mill certificate.
How to choose a spring material
- Temperature: above about 120 °C, move from carbon wire to chrome-vanadium, chrome-silicon or stainless.
- Corrosion: start with stainless, or use carbon steel with a suitable finish where the environment is mild.
- Fatigue: chrome-silicon and shot peening help under high stress and many cycles.
- Electrical: phosphor bronze or beryllium copper when the spring also conducts current.
- Cost: music wire and hard-drawn wire are the economical starting point at room temperature.
Wanjin agrees the material grade for each project against the drawing and the operating conditions. The calculator includes the moduli above, and you can send your requirements for a material review.
Key Takeaways
- Stress, temperature and corrosion decide the material.
- Stainless 302/304 has about 13% lower shear modulus than carbon spring steel, so the same geometry gives about 13% less rate.
- Equivalent grades are close, not identical; confirm against the mill certificate.